Nov 10 2026
/
H13 vs 1.2344 vs SKD61 vs 4Cr5MoSiV1
1. Introduction
H13 (AISI), 1.2344 (DIN), SKD61 (JIS), and 4Cr5MoSiV1 (GB) all belong to the chromium-molybdenum-vanadium hot work tool steel family. They offer excellent hot strength, thermal fatigue resistance, and hardenability, and are widely used in aluminum die casting dies, hot forging dies, and extrusion tooling.
This document systematically compares the equivalent grade relationships, chemical composition differences, effects of melting routes on performance, and purchasing considerations for design engineers and procurement teams.
2. Equivalent Grade Comparison
| Standard System | Standard | Grade |
|---|---|---|
| USA | AISI | H13 |
| Germany | DIN | 1.2344 |
| Japan | JIS | SKD61 |
| China | GB | 4Cr5MoSiV1 |
3. Chemical Composition Comparison
| Element (wt%) | AISI H13 | DIN 1.2344 | JIS SKD61 | GB 4Cr5MoSiV1 |
|---|---|---|---|---|
| C | 0.32–0.45 | 0.35–0.42 | 0.35–0.42 | 0.32–0.42 |
| Si | 0.80–1.25 | 0.80–1.20 | 0.80–1.20 | 0.80–1.20 |
| Mn | 0.20–0.60 | 0.25–0.50 | 0.25–0.50 | 0.20–0.50 |
| P ≤ | 0.030 | 0.030 | 0.030 | 0.030 |
| S ≤ | 0.030 | 0.020 | 0.020 | 0.020 |
| Cr | 4.75–5.50 | 4.80–5.50 | 4.80–5.50 | 4.75–5.50 |
| Mo | 1.10–1.75 | 1.20–1.50 | 1.00–1.50 | 1.10–1.75 |
| V | 0.80–1.20 | 0.85–1.15 | 0.80–1.15 | 0.80–1.20 |
4.H13 vs 1.2344 vs SKD61 vs 4Cr5MoSiV1
AISI H13 : Widest chemical composition range, sulfur capped at 0.030%, upper-tier toughness slightly lower. Mature supply chain in North America, strongest general-purpose suitability. Typically used for general hot forging dies and non-critical die casting applications. Offers the most cost flexibility.
DIN 1.2344 : Tighter vanadium ranges, sulfur ≤ 0.020%. The strictest composition tolerances of the four standards. Better hot hardness and resistance to dimensional sag under load. Preferred by European customers; suited for heavy-duty extrusion and high-pressure aluminum die casting dies.
JIS SKD61 : Sulfur capped at ≤ 0.020%, with a lower molybdenum floor. Balanced toughness and thermal fatigue resistance, consistent polishability. Widely traded in Southeast Asia, Japan and Korea. Mainstay for small-to-medium aluminum and zinc die casting dies.
GB 4Cr5MoSiV1 : Chinese equivalent grade to H13, composition range aligned with ASTM H13, sulfur ≤ 0.020%. Abundant domestic supply, high cost-performance ratio. The most common grade for domestic die casting and hot forging tooling.
5. Typical Applications
- Aluminum die casting dies
- Zinc die casting dies
- Hot forging dies
- Extrusion dies
- Hot shear blades